A torch moves along the joint of two 16 mm S355 plates. The simulation follows the heat into the steel: the melt pool, the highest temperature each point reaches and how fast it cools again. That cooling time decides the microstructure in chapter 2.

Talk to us
Two steel plates welded by a moving torch; the temperature on the surface trails behind the arc
7.2 kW at 300 mm/min, 1.44 kJ/mm: the temperature on every surface, white above the melting point
  • 2520 °CHottest point, in the melt pool under the arc
  • 12 × 5.6 mmWidth and depth of the molten zone
  • 8.65 sFrom 800 to 500 °C next to the fusion line; EN 1011-2 gives 9.2 s
  • 62 °CWarmest point 30 minutes after the arc stops

The section · x = 76 mm

The highest temperature each point ever saw.

Halfway along the weld, across the top face. Where the curve crosses a transformation temperature, the steel changes for good: these crossings are the zone boundaries of chapter 2.

Peak temperature, top face · dashed: temperatures where the steel changes

  • Fusion zone0–5 mm · above 1500 °C
  • Coarse-grain HAZto 6 mm · above 1100 °C
  • Fine-grain HAZto 7 mm · above Ae3 837 °C
  • Intercritical HAZto 8 mm · above Ae1 715 °C
  • Base metalbeyond · below Ae1

The heat-affected zone is only about 3 mm wide on the surface: the grid of the model is 1 mm, so the zone edges are read to the nearest millimetre.

Cooling time t8/5 · against the standard

8.65 s from the model. 9.2 s from EN 1011-2.

Welding standards judge a procedure by the time the heat-affected zone takes to cool from 800 to 500 °C. EN 1011-2 has a formula for it. The model computes it at every point along the weld.

t8/5 next to the fusion line, along the weld EN 1011-2, thin plate (2D) thick plate (3D)

Model, x = 76 mm
8.65 s
EN 1011-2, thin plate
9.2 s
EN 1011-2, thick plate
7.6 s

Below a transition thickness of 17.6 mm the standard uses the thin-plate formula, so for 16 mm it predicts 9.2 s; the model is 6 % shorter, between the two formulas. Near the start and the end of the weld the plate around the arc is colder and t8/5 drops to about 3 s: the formula cannot show this, the model can.

Inputs · every value has an origin

What is standard, and what is assumed.

There was no real weld to start from, so the process values are typical ones. With a welding procedure and a macro section of a real weld, the heat source is calibrated instead.

  1. assumedWelding process
    • 30 V · 300 A · 300 mm/min
    1.44 kJ/mm with the arc efficiency, typical values for one MAG pass
  2. standardArc efficiency
    • k = 0.8
    Share of the arc power that enters the plates
  3. assumedHeat-source shape
    • 6 / 12 / 7 / 6 mm
    Double-ellipsoid source: front, rear, half width, depth. Not yet calibrated against a macro section
  4. standardThermal properties of the steel
    • λ(T), c(T), ρ 7850 kg/m³
    Temperature-dependent conductivity and heat capacity, with the 735 °C peak of c
  5. assumedMelting
    • 270 kJ/kg · 1450–1500 °C · λ ×4
    Latent heat and a higher conductivity in the melt pool for the flow it does not model
  6. standardSurface
    • ε 0.7 · film 10 W/m²K (assumed) · 20 °C
    Radiation and convection on every free face

How it works

Three steps, each one a script you can rerun.

  1. 1 · Model

    Half the joint, 1 mm grid at the weld

    69 309 points. The joint line is a plane of symmetry, so one plate stands for both.

  2. 2 · Heat source

    A double ellipsoid that moves

    7.2 kW spread over the arc's footprint, 130 mm in 26 s, then 30 minutes of cooling in air.

  3. 3 · Solve

    Melting and properties that change with temperature

    272 time steps from 0.2 s, about 8 minutes. The temperature of every point at every step is stored for chapter 2.

The evidence

Every number comes with its check.

The energy has to add up, an independent solver has to agree, and a finer grid or a shorter time step must not change the answer.

Decision dossierWeld thermal
  • Heat stored + lost against heat put incloses to < 0.001 %
  • Cooling time 800 → 500 °C against EN 1011-2 (thin plate)8.65 s vs 9.2 s
  • Linear version against CalculiXpeaks within 2 %, t8/5 7.86 vs 7.85 s
  • Time step halvedpeaks ≤ 1.7 %, t8/5 0.5 %
  • Grid 2 mm → 1 mmlargest change 2.0 %
  • Melt-pool conductivity ×2 instead of ×4t8/5 in the HAZ changes 3 %

Assumptions: one MAG pass with 30 V, 300 A and 300 mm/min (typical values), arc efficiency 0.8 (standard), double-ellipsoid heat source 6/12/7/6 mm (assumed, not calibrated), power ramped up over the first second. Thermal properties of the steel from the standard for steel structures in fire, latent heat and the higher conductivity of the melt pool assumed. Butt joint without groove or filler metal. Convection 10 W/m²K (assumed), emissivity 0.7 (standard), 20 °C around. The melt-pool peak depends on the melt-pool conductivity; the heat-affected zone hardly does (3 %).

Pilot partners wanted

Have a welding procedure to check before the first trial? Let's simulate it.

SPDM Tech is in its build-up phase. As one of the first pilot partners, you bring one real question, from a circuit board, a drawing or a simulation process, and get a checked answer.

Become a pilot partner